No passwords, No popups, No cost, No AI:
we earn from 'affiliate link' purchases, making the site possible

Home /
T.O.C.
Fun
FAQs
Good
Books
Ref.
Libr.
Adver-
tise
Help
Wanted
Current
Q&A's
Site 🔍
Search
ted_yosem
Sound technical content, curated with aloha by
Ted Mooney, P.E. RET
Pine Beach, NJ
finishing.com -- The Home Page of the Finishing Industry

  The authoritative public forum
  for Metal Finishing since 1989
  mfhotline


  -----

Arsenic Plating




2006

Dear All

We need the best method for plating Arsenic (As+3) from solution as element. It would be appreciated any help.

Best regards,

Reza Alizadehfard
MITPL - Perth, Australia


Ed. note: your question could probably be answered best if you described the specifics of your situation instead of casting your question in the abstract, Reza.


2006

Arsenic plating:
100 gm arsenic acid
30 gm sodium carbonate this on eBay or Amazon] (calc.)
10 gm potassium cyanide
1 lit water
charcoal anodes(in silk bags)
0,4 A/dm2
15-20 °C temp.
Very toxic stuff-avoid any contact with solution,objects must be oxide and grease free!
According to W.Machu:Metallische Ueberzuege,Leipzig 1948.

Goran Budija
- Cerovski vrh Croatia




(No "dead threads" here! If this page isn't currently on the Hotline your Q, A, or Comment will restore it)

Q, A, or Comment on THIS thread -or- Start a NEW Thread

Disclaimer: It's not possible to fully diagnose a finishing problem or the hazards of an operation via these pages. All information presented is for general reference and does not represent a professional opinion nor the policy of an author's employer. The internet is largely anonymous & unvetted; some names may be fictitious and some recommendations might be harmful.

If you are seeking a product or service related to metal finishing, please check these Directories:

Finishing
Jobshops
Capital
Equipment
Chemicals &
Consumables
Consult'g,
& Software


About/Contact  -  Privacy Policy  -  ©1995-2024 finishing.com, Pine Beach, New Jersey, USA  -  about "affil links"